我们展示了与后段制程(BEOL)兼容的增强型(E-mode)非晶氧化物半导体(AOS)场效应晶体管(FET)所实现的创纪录逻辑性能。这些器件在沟道长度(Lch)缩小到40 nm时仍表现出接近理想的可微缩性。采用等离子体增强原子层沉积(PEALD)生长的In2O3沟道,我们在Lch = 40 nm器件中实现了增强型工作:在漏源电压(Vds)为0.5 V时,最大驱动电流(Imax)达1.35 mA/µm,峰值跨导(gm,peak)达490 µS/µm,室温平均亚阈值摆幅(Savg)为63 mV/dec,接近热力学极限。我们演示了169 Ω·µm的源漏总电阻(Rsd),为增强型AOS-FET中的最低纪录。电容-电压(C-V)特性揭示了本征沟道区与源漏/栅交叠区具有不同的阈值电压(Vt)。我们建立了基于物理的MVS-AOS模型,能够准确刻画实验器件中的关键物理机制,包括源漏区电容的频率色散。本工作推动了BEOL AOS-FET技术的最新进展,并为该器件平台在BEOL单片三维集成中的设计-工艺协同优化(DTCO)铺平了道路。
We demonstrate record logic performance in backend-of-the-line (BEOL)-compatible enhancement-mode (E-mode) amorphous oxide semiconductor (AOS) field-effect transistors (FETs). These devices exhibit near-ideal scalability down to 40 nm in channel length (Lch). Using an In2O3 channel by plasma-enhanced atomic-layer deposition (PEALD), we achieve E-mode operation in Lch = 40 nm devices with a maximum drive current (Imax) of 1.35 mA/µm, a peak transconductance (gm,peak) of 490 µS/µm, and a close-to-thermal-limit average room-temperature subthreshold swing (Savg) of 63 mV/dec, all at a drain-to-source voltage (Vds) of 0.5 V. A total source (S) and drain (D) resistance (Rsd) of 169 Ω.µm, record-low among E-mode AOS-FETs, is demonstrated. Capacitance-voltage (C-V) characteristics reveal different threshold voltages (Vt) in the intrinsic channel and in the S/D to gate (G) overlap regions. We develop a physics-based MVS-AOS model which accurately captures the essential physics at play in our experimental devices, including C with frequency dispersion in the S/D region. This work advances state-of-the-art BEOL AOS-FET technology, and paves the way for future design-technology co-optimization (DTCO) on this promising device platform for BEOL monolithic 3D integration.
| 指标 | 数值 | 说明 |
|---|---|---|
| 最大驱动电流 Imax | 1.35 mA/µm @ Vds = 0.5 V(Vds = 0.7 V 时 1.9 mA/µm) | W/Lch = 60/40 nm 器件,为E-mode AOS-FET最高纪录 |
| 峰值跨导 gm,peak | 490 µS/µm @ Vds = 0.5 V | W/Lch = 60/40 nm 器件中测得 |
| 平均亚阈值摆幅 Savg | 63 mV/dec(Lch = 40 nm);长沟道 60 mV/dec | 接近室温热力学极限,三个电流数量级内保持 |
| 源漏总电阻 Rsd | 169 Ω·µm | W = 60 nm 时提取,E-mode AOS-FET 中最低,对应转移长度 LT ≈ 30 nm |
| 电容等效厚度 CET | ~1.4 nm | 由不同 Lch 器件间的归一化微分电容 Cdiff 提取 |
| 栅介质/沟道厚度 | HfO2 4.8 nm / In2O3 2.3 nm | PEALD 250 °C 栅介质、150 °C 沟道,W 栅金属 |
Imax = 1.35 mA/µm @ Vds = 0.5 V;Rsd = 169 Ω·µm(E-mode AOS-FET 最低)
原子层沉积(ALD)、低温工艺、图案化与光刻
BEOL单片3D集成、嵌入式DRAM(eDRAM)、DTCO设计工艺协同优化