WaytoICT › 香农学术库 › IEDM 2025 › 论文

原子层沉积非晶锗掺杂氧化铟及其迁移率—稳定性—抗结晶性权衡的提升

Atomic Layer Deposited Amorphous Ge-Doped Indium Oxide with Enhanced Mobility–Stability–Crystallization Resistance Tradeoff
新型沟道与材料器件氧化物半导体FET薄膜晶体管(TFT)DRAM单元互连/BEOL氧化物半导体(IGZO/ITO)硅基CMOS实验+仿真
IEDM 2025University of Notre Dame
采用ALD制备非晶Ge掺杂In2O3沟道,兼顾迁移率、偏压稳定性与抗结晶性,迁移率达42 cm²/V·s、SS约60 mV/dec,可统一BEOL逻辑与1T1C DRAM热预算需求。

基本信息

作者
YuShan Lee1*, Xingtian Wang1*, Jiahui Duan1*, Guanyu Zhou1, Md Abdullah Al Mamun2, Yiyan Yu1, Pengyu Ren1, Sizhe Ma1, Shan Deng1, Zijian Zhao1, Yixin Qin1, Alessandra Leonhardt3, Serges Zambou3, Aditya Chauhan3, Ranjith Ramachandran3, Glen Wilk4, Xiao Gong5, Kyeongjae Cho2, Christopher Hinkle1, and
机构
University of Notre Dame
国家
美国
会议
IEDM 2025(International Electron Devices Meeting)
供电电压
VD = 1 V、VOV = 1 V(导通特性);栅过驱动应力 VOV = ±2 V
工作温度
室温(电学与BTI测试);退火温度 500–800 °C

摘要

本文展示了锗掺杂氧化铟(Ge:In2O3)作为一种有前景的氧化物半导体材料的潜力,其在迁移率、电学稳定性与抗结晶能力之间取得了更优的权衡。这使其既适用于低于400 °C的背面互连(BEOL)单片三维集成,也适用于高于500 °C的1T1C DRAM工艺。通过与硅掺杂In2O3(Si:In2O3)的对比研究,我们表明:(i) 更离域的Ge 4s轨道相比Si掺杂带来更高的电子迁移率,这一结论得到第一性原理计算与实验结果的共同支持,在1:5的Si:In与Ge:In掺杂比下迁移率分别为21 cm²/V·s和42 cm²/V·s;(ii) 强的Ge–O与Si–O键分别将氧空位形成能提高约0.4 eV和约1 eV,从而同时增强偏压稳定性与抗结晶能力——两种薄膜在500 °C长时间退火后仍保持非晶态,其中Si:In2O3在高达800 °C时仍稳定;(iii) 器件表现出优异性能,亚阈值摆幅约60 mV/dec,开/关比约10^10,开态电流为150 μA/μm(Si:In2O3)和330 μA/μm(Ge:In2O3)(VOV=1 V,VD=1 V);(iv) 即使采用超薄(5–10 nm)栅介质,两种沟道在±2 V过驱动应力下经过1000 s后仍保持|ΔVTH| < 100 mV的高可靠性。这些结果确立了ALD生长的Ge:In2O3作为一种通用氧化物半导体平台,能够在先进单片三维集成方案中统一BEOL逻辑与FEOL DRAM的需求。

Abstract

In this work, we demonstrate the potential of germanium-doped indium oxide (Ge:In2O3) as a promising oxide semiconductor offering an improved tradeoff among mobility, electrical stability, and crystallization resistance. This makes it suitable for both <400 °C back-end-of-line (BEOL) monolithic 3D integration and >500 °C 1T1C DRAM process. Through a comparative study with silicon-doped In2O3 (Si:In2O3), we show that: (i) the more delocalized Ge 4s orbitals yield higher electron mobility compared to Si doping, supported by first-principles calculations and experimental results, with mobilities of 21 cm2/V·s and 42 cm2/V·s for 1:5 Si:In and Ge:In doping ratios, respectively; (ii) strong Ge–O and Si–O bonds raise the oxygen vacancy formation energy by ~0.4 eV and ~1 eV, respectively, enhancing both bias stability and crystallization resistance—both films remain amorphous after a 500 °C prolonged anneal, with Si:In2O3 stable even up to 800 °C; (iii) devices exhibit excellent performance, with subthreshold swing ~60 mV/dec, ON/OFF ratio ~1010, and ON currents of 150 μA/μm (Si:In2O3) and 330 μA/μm (Ge:In2O3) VOV=1V, VD=1V; (iv) both channels show high reliability with |ΔVTH| < 100 mV under ±2 V overdrive stress for 1000 s, even with ultra-thin (5–10 nm) gate dielectrics. These results position ALD-grown Ge:In2O3 as a versatile oxide semiconductor platform capable of unifying BEOL logic and FEOL DRAM requirements in advanced monolithic 3D integration schemes.

关键技术指标

指标数值说明
场效应迁移率 μFE42 cm²/V·s1:5 Ge:In ALD循环比下的峰值迁移率,约为同比例Si掺杂(21 cm²/V·s)的3倍
开态电流 ION330 μA/μmGe:In2O3器件在VOV=1 V、VD=1 V下的开态电流,Si:In2O3为150 μA/μm
亚阈值摆幅 SS~60 mV/decGe:In比例为1:3与1:5时均保持陡峭开关特性
开/关电流比~10^10器件转移特性中的开关比
偏压温度不稳定性|ΔVTH| < 100 mV±2 V过驱动应力1000 s后阈值漂移,栅介质仅5–10 nm
抗结晶温度600 °C(Ge:In=1:5)/ 800 °C(Si:In=1:5)长时间退火后仍保持非晶结构的最高温度

性能概述

场效应迁移率 42 cm²/V·s(Ge:In=1:5);开态电流 330 μA/μm(VOV=1 V,VD=1 V)

技术路线

原子层沉积(ALD)、低温工艺、热稳定性、单片3D集成、BTI

应用场景

单片3D集成、BEOL逻辑、1T1C DRAM