传统 Si 沟道铁电场效应晶体管(FEFET)的耐久性退化主要由界面 SiO2(IL)层内的陷阱产生所主导,其中升高的电场会加速缺陷产生,导致极化屏蔽以及存储窗口(MW)的逐步塌陷。在本工作中,我们证明:利用 scavenging 减薄 IL 层会形成具有更高电容的亚化学计量 SiOx,从而显著改善 FEFET 的耐久特性。这种 IL 工程带来电压的重分布,并使 FEFET 失效转变为由下方铁电(FE)层而非 IL 主导的新模式。这种 FE 主导的退化范式带来三项关键优势:(1) 通过最小化界面态积累抑制亚阈值摆幅(SS)恶化;(2) 在长程循环中 MW 保持稳定,表现为直至 FE 击穿前高 VTh 与低 VTh 态均保持稳定;(3) 由于 IL 层陷阱去俘获更快,读后写延迟降低。我们还演示了在 125 ℃ 下具有 10^4 次循环耐久性和低 SS 的稳健 MW。此外,我们使用 GinestraTM 仿真量化了 IL 与 FE 层中的陷阱产生和电场。这些发现确立了一条通过 IL 工程驱动铁电退化控制来实现高耐久、稳定 VTh FEFET 的创新且高效途径。
Endurance degradation in conventional Si-channel ferroelectric FETs (FEFETs) is predominantly governed by trap generation within the interfacial SiO2 (IL) layer, where elevated electric fields accelerate defect generation, leading to polarization screening and progressive memory window (MW) collapse. In this work, we demonstrate that using scavenging to thin the IL layer induces a sub-stoichiometric SiOx, with higher capacitance which dramatically improves the endurance characteristics of the FEFET. This IL engineering results in a redistribution of voltage and a new mode of FEFET failure driven by the underlying FE rather than the IL. This FE-driven degradation paradigm yields three critical advantages: (1) suppression of subthreshold slope (SS) deterioration by minimizing interface state buildup, (2) MW stability over extended cycling, as evidenced by a stable high-VTh and low-VTh states until FE breakdown, and (3) reduction in read-after-write latency due to faster de-trapping of traps in IL layer. We also demonstrate robust MW at 125 °C with 10^4 cycles endurance and low SS. Further, we quantify trap generation and electric fields in the IL and FE layers using GinestraTM simulations. These findings establish an innovative and efficient pathway to high endurance, stable VTh FEFETs via the implementation of an IL engineering-driven control of ferroelectric degradation.
| 指标 | 数值 | 说明 |
|---|---|---|
| 存储窗口(MW) | 0.5 V | scavenged 器件在 200 ns 写脉冲、3.5 V 写电压下的存储窗口 |
| 耐久性 | 10^4 次循环 @125 ℃ | bipolar 应力循环下 MW 稳定保持至铁电层击穿 |
| 等效氧化层厚度(EOT) | 1.25 nm | scavenged 器件 EOT,低于未 scavenging 器件的 1.58 nm |
| 亚阈值摆幅退化 | 1.25 倍 | 循环后 SS 仅增大 1.25 倍,标准器件为 3.3 倍 |
| 读后写延迟 | 降低约两个数量级 | scavenged 器件在低两个数量级的读后写延迟下即实现 MW 完全恢复 |
| 写电压 | 3.5 V | 达到同等 MW 所需写电压,标准器件需 4.5 V |
125 ℃ 下 10^4 次循环耐久性;0.5 V 存储窗口 @ 3.5 V/200 ns 写脉冲
铁电极化、电荷俘获、高k金属栅、热稳定性、失效分析
嵌入式非易失存储、存内计算、高温电子