我们通过实验在TSMC N40 CMOS代工芯片上演示了采用ALD掺钨氧化铟(IWO)沟道的双栅(DG)非易失电容存储器(nvCAP)的单片三维(M3D)集成。关键技术进展包括:i) 提出新型nvCAP双栅工程,有效解决氧化物沟道铁电体擦除弱与保持性差的问题;ii) 首次在代工厂CMOS芯片上成功实现DG nvCAP的后道(BEOL)集成,在Vread=0 V下获得约64.4的非破坏性电容开关比,为已报道BEOL兼容nvCAP中的最高纪录;iii) 在BEOL集成的DG nvCAP中实现|Vread|=1 V下超过10^9次的非破坏性读耐久;iv) 提出M3D非破坏性“电容型”数字存内计算(Cap-DCIM)范式,相比领先的模拟CIM实现146倍更优的品质因数(TOPS/W×TOPS/mm2),相比SRAM基DCIM静态功耗低111倍——这得益于高可扩展的数字逻辑与DG nvCAP的BEOL集成。最后,我们通过在代工CMOS芯片上单片集成DG nvCAP,演示了BEOL电容调制FEOL硅晶体管电流放大的过程,从而实验验证了M3D Cap-DCIM的工作原理。这些进展为克服现有模拟CIM方法长期存在的可扩展性与变异度限制提供了一条有前景的路径。
We experimentally demonstrate monolithic 3D (M3D) integration of dual-gated (DG) non-volatile capacitive memory (nvCAP) featuring an ALD W-doped In2O3 (IWO) channel on a TSMC N40 CMOS foundry chip. Key technical advancements include: i) Novel dual-gate engineering of nvCAP, effectively addressing the weak erase and poor retention challenges with oxide-channel ferroelectrics; ii) First successful BEOL integration of DG nvCAP on a foundry CMOS chip, achieving a non-destructive capacitive on/off ratio of ~64.4 at Vread=0 V—a record among reported BEOL-compatible nvCAPs; iii) Non-destructive read endurance exceeding 109 cycles at |Vread|=1 V, achieved in BEOL-integrated DG nvCAPs; iv) Introduction of the M3D non-destructive "capacitive" digital-compute-in-memory (Cap-DCIM) paradigm, achieving 146× higher figure-of-merit (TOPS/W×TOPS/mm2) compared to leading analog CIMs and 111× lower static power versus SRAM-based DCIMs—enabled by highly scalable digital logic and BEOL integration of DG nvCAPs. Finally, we experimentally validate the operational principle of M3D Cap-DCIM, by demonstrating BEOL capacitance-modulated FEOL Si transistor current amplification through monolithically integrated DG nvCAP on a foundry CMOS chip. These advancements offer a promising pathway to overcome the long-standing scalability and variability limitations of leading analog CIM approaches.
| 指标 | 数值 | 说明 |
|---|---|---|
| 非破坏性电容开关比 Con/Coff | ~64.4 @ Vread=0 V | BEOL集成的双栅nvCAP在零读出电压下的电容开/关比,为BEOL兼容nvCAP最高纪录 |
| 非破坏性读耐久 | >10^9 cycles @ |Vread|=1 V | BEOL集成DG nvCAP在1 V读电压下的读取循环次数 |
| 保持特性(Retention) | >10^4 s @25 °C;10^3 s @85 °C | 较既有工作提升10倍以上的电容态保持时间 |
| 铁电剩余极化 2Pr | ~34.6 μC/cm2 | BE/7 nm HZO/3.5 nm IWO/TE 电容经450 °C/15 min退火后的P-V特性 |
| 品质因数 FOM (TOPS/W×TOPS/mm2) | 146× (对比22nm RRAM基ACIM);静态功耗低111× (对比SRAM基DCIM) | 基于实测数据校准的电路模型在3nm节点下的PPA投影 |
电容开关比 Con/Coff ~64.4 @ Vread=0 V;非破坏性读耐久 >10^9 cycles @ |Vread|=1 V
单片3D集成、原子层沉积(ALD)、铁电极化、存内计算
数字存内计算(DCIM)、AI加速器、先进逻辑三维集成
打开交互版 · AI 解读 / 同类对比 / 完整指标在香农学术库中查看(需会员)