我们演示了在AlN衬底上用MOVPE生长的低电阻、高击穿场且无电流崩塌的AlN/GaN/AlN HEMT。基于TEGa的生长降低了碳杂质,提升了二维电子气密度与迁移率。对AlN势垒进行简单凹槽刻蚀可降低接触电阻。采用应力调控的SiN进行表面钝化,在不降低迁移率、不增加栅漏电的前提下抑制了表面陷阱。该完全应变异质结的穿透位错密度低于10^4 cm−2,支撑了稳健的动态工作。这些结果证实了MOVPE用于可规模化、高性能超宽禁带器件的可行性。
We demonstrate low-resistance, high-breakdown field, and current-collapse-free AlN/GaN/AlN HEMTs grown by MOVPE on AlN substrates. TEGa-based growth reduces carbon impurities, enhancing 2DEG density and mobility. Simple recess etching of the AlN barrier enabled reducing contact resistance. Surface passivation with stress-engineered SiN suppressed surface traps without degrading mobility and increasing gate leakage. The fully strained heterostructure with threading dislocation density below 104 cm−2 supports robust dynamic operation. These results confirm MOVPE's viability for scalable, high-performance of ultra-wide bandgap devices.
| 指标 | 数值 | 说明 |
|---|---|---|
| 二维电子气密度 | 2.3×10^13 cm−2 | TEGa生长样品#2,较TMGa样品#1(1.1×10^13 cm−2)显著提升 |
| 薄层电阻 | 507 Ω/sq | TEGa生长样品#2的霍尔测试薄层电阻 |
| 接触电阻 | 2.4 Ω·mm | 样品#2经8 nm凹槽刻蚀后的TLM接触电阻(未刻蚀为64 Ω·mm) |
| 导通电阻 | 8.0 Ω·mm | 栅长2 μm器件的RON,结合低薄层电阻与低接触电阻实现 |
| 击穿场 | 2 MV/cm | 未钝化样品的FBD = VBD/LGD,约为常规GaN沟道HEMT的两倍 |
| 最大漏极电流密度 | 0.43 A/mm | 样品#2的Imax;关态漏电<1 μA/mm |
击穿场 2 MV/cm;导通电阻 RON = 8.0 Ω·mm(比导通电阻 RONA 改善约两个数量级)
外延生长、选择性刻蚀、应变工程
高功率电子、高频器件、功率开关