本工作报道了等效氧化层厚度(EOT)微缩的MoS₂沟道直接生长二维(2D)场效应晶体管(FET)。我们提出了一种稳健的器件制造工艺,引入氧化物钝化步骤以利用直接生长的二维沟道。该新工艺方案使200 mm晶圆上直接生长二维FET的器件良率接近100%,并获得洁净的接触区域。与转移器件相比,直接生长器件实现了更低的界面缺陷态密度(Dit),从而减小了器件波动。此外,我们在直接生长MoS₂过程中以Al掺杂HfO₂(HfAlO)和ZrO₂作为衬底,对栅介质的晶体结构进行工程调控。通过优化器件制造工艺与介质,我们在EOT为1.15 nm时实现了已报道直接生长二维FET中最高的开态电流(ION)820 μA/μm。
This work reports on equivalent oxide thickness (EOT)-scaled MoS₂ channel direct-grown two-dimensional (2D) field-effect transistors (FETs). We introduce a robust device fabrication process that integrates an oxide passivation step to utilize direct-grown 2D channels. The new process scheme enables nearly 100% device yield on 200 mm wafers for direct-grown 2D FETs and clean contact areas. From directly grown devices, we achieve lower interface defect states (Dit) than transferred devices, reducing device variation. Moreover, we engineer the crystal structure of the gate dielectrics using Al-doped HfO₂ (HfAlO) and ZrO₂ as substrates during direct MoS₂ growth. By optimizing the device fabrication process and dielectrics, we achieve the highest reported on-current (ION) of 820 μA/μm at EOT of 1.15 nm among direct-grown 2D FETs.
| 指标 | 数值 | 说明 |
|---|---|---|
| 开态电流 ION | 820 μA/μm @ EOT 1.15 nm | 已报道直接生长二维FET中的最高开态电流 |
| 等效氧化层厚度 EOT | 1.33 nm(5 nm HfAlO);器件演示 1.15 nm | 晶化HfAlO介电常数提升至14.66,实现5 nm厚度下的EOT微缩 |
| 界面陷阱密度 Dit | 0.4–1.1×10¹² cm⁻²/eV(直接生长)vs 0.7–2.3×10¹² cm⁻²/eV(转移) | 电导法测得,直接生长界面质量优于转移界面 |
| 器件良率 | 近100%(624个器件,200 mm晶圆) | 直接生长多晶MoS₂沟道器件的一致性验证 |
| 特性变异系数 C.V. | ION 8.4%、VTH 8.2% | 多晶沟道与二维/介质界面在片内具有均匀质量 |
| 介电常数 k | 14.66 | Al掺杂使HfAlO由单斜相转为四方相并提高介电常数 |