4H-SiC器件通常因衬底电阻的限制而被认为在低压应用中缺乏竞争力。本工作挑战这一长期观点,展示了一种新型150 mm单晶4H/3C-SiC工程衬底,其电阻率比常规4H-SiC低45倍以上。该工程衬底利用3C-SiC的超低电阻率,并通过集成约580 nm的顶级质量4H-SiC模板来克服其高缺陷密度。该模板通过表面活化键合与离子剥离转移到液相生长的3C-SiC衬底上。获得了陡峭、无缺陷的键合界面,其势垒低于30.4 mV,热边界电阻达到创纪录的1 + 0.7/–0.6 m²·K/GW。在该衬底上制作的200 V肖特基势垒二极管(SBD)展现出创纪录的低比导通电阻(Ron,sp)0.50 mΩ·cm²以及超过300 A的浪涌电流耐受能力——相比在4H-SiC衬底上制作的相同器件,Ron,sp降低47%,浪涌电流鲁棒性提升20%。这些结果建立了一个可规模化的异质集成材料平台,可支撑下一代低压SiC功率电子器件。
4H-SiC devices are usually considered uncompetitive for low-voltage applications due to substrate resistance limitations. This work challenges this long-held belief by demonstrating a novel 150 mm single-crystal 4H/3C-SiC engineered substrate with resistivity over 45× lower than conventional 4H-SiC. The engineered substrate leverages the ultra-low resistivity of 3C-SiC and overcomes its high defect density by integrating a ~580 nm prime-grade 4H-SiC template. This template is transferred via surface-activated bonding and ion-cut onto a liquid-phase-grown 3C-SiC substrate. A sharp, defect-free bonding interface was achieved with a potential barrier below 30.4 mV and a record thermal boundary resistance of 1 + 0.7/–0.6 m²·K/GW. 200 V Schottky barrier diodes (SBDs) fabricated on this substrate demonstrate a record low specific on-resistance (Ron,sp) of 0.50 mΩ·cm² and a surge current tolerance over 300 A—representing a 47% reduction in Ron,sp and a 20% increase in surge current robustness compared to identical devices fabricated on 4H-SiC substrates. The results establish a scalable hetero-integration material platform for enabling next-generation low-voltage SiC power electronics.
| 指标 | 数值 | 说明 |
|---|---|---|
| 衬底电阻率 | 0.39 mΩ·cm | 涡流法测得,仅比3C-SiC衬底高0.01 mΩ·cm,比常规4H-SiC(15–20 mΩ·cm)低45倍以上 |
| 比导通电阻Ron,sp | 0.50 mΩ·cm² | 200 V SBD上测得,相比4H-SiC衬底同类器件降低47% |
| 浪涌电流耐受 | >300 A | 相比4H-SiC衬底同类器件提升20%的浪涌鲁棒性 |
| 键合界面势垒 | <30.43 mV | EFM测得界面峰值电场仅1.05 kV/cm,利于电子隧穿导通 |
| 热边界电阻TBR | 1 +0.7/–0.6 m²·K/GW | TTR法提取,为4H-SiC键合体系报道最低值之一,NEMD仿真得0.45 m²·K/GW |
| 键合率 | 87% | 100 keV H⁺注入、Ar离子束表面活化后室温键合并在>850 ℃退火剥离获得 |
比导通电阻Ron,sp = 0.50 mΩ·cm²;衬底电阻率 0.39 mΩ·cm(比常规4H-SiC低45倍以上)
晶圆键合、转移与剥离、外延生长、热稳定性
低压SiC功率器件、电动汽车、可再生能源与工业驱动
打开交互版 · AI 解读 / 同类对比 / 完整指标在香农学术库中查看(需会员)