我们报道,赝形HfO2-TiO2-HfO2(HTH)插层通过稳定6 nm厚萤石相Hf0.5Zr0.5O2(HZO)的亚稳正交(o)相,克服了其本征铁电限制。HfO2与TiO2之间原子尺度的晶格匹配(3.6–3.7 Å)促进共格生长,使o相晶粒增大(>25 nm),并使畴能垒降低72%。畴动力学与低频噪声分析揭示了翻转效率的提升和畴取向的均匀性,证实了赝形模板化的贡献。HTH-HZO实现了创纪录的剩余极化(2Pr)133 μC/cm²和超低矫顽场1.17 MV/cm,优于萤石基铁电体并达到PZT的效率水平。在FeCap工作中,器件在0 V读取偏置下表现出9.6的电容存储窗口(CMWε),并在10^10次循环后仍保持7.7。采用实测FeCap参数进行的BNN仿真相比软件基线取得了高推理精度,展示了其在低功耗、CMOS兼容存储与神经形态系统中的潜力。
We report that a pseudomorphic HfO2-TiO2-HfO2 (HTH) interlayer overcomes the intrinsic ferroelectric (FE) limitations of 6nm thick fluorite Hf0.5Zr0.5O2 (HZO) by stabilizing its metastable orthorhombic (o-) phase. Atomic-scale lattice alignment between HfO2 and TiO2 (3.6–3.7 Å) promotes coherent growth, enlarging o-phase grains (>25 nm) and reducing domain energy barriers by 72%. Domain dynamics and low-frequency noise analysis reveal enhanced switching efficiency and uniform domain alignment, confirming the contribution of pseudomorphic templating. HTH-HZO achieves a record remnant polarization (2Pr) of 133 μC/cm2 and an ultralow coercive field of 1.17 MV/cm, outperforming fluorite-based FEs and matching PZT efficiency. In FeCap operation, the device shows a capacitive memory window (CMWε) of 9.6 at 0 V read bias and retains 7.7 after 1010 cycles. BNN simulations using measured FeCap parameters achieve high inference accuracy compared to software baselines, demonstrating potential for low-power, CMOS-compatible memory and neuromorphic systems.
| 指标 | 数值 | 说明 |
|---|---|---|
| 剩余极化 2Pr | 133 μC/cm² | 6 nm HZO铁电电容器中创纪录的剩余极化,优于以往萤石基铁电体 |
| 矫顽场 Ec | 1.17 MV/cm | 6 nm厚度下达到PZT级低矫顽场,远低于常规HZO的2–3 MV/cm |
| 电容存储窗口 CMWε | 9.6 @ 0 V | 0 V读取偏置下的相对介电常数电容存储窗口,为对照样品的3.7倍 |
| 循环保持能力 | CMWε 7.7 @ 10^10 循环 | FeCap经10^10次循环应力后仍保持较稳定的电容存储窗口 |
| 畴翻转势垒 UB | 降低 72% | 相比SiO2-HZO对照样品势垒能量显著降低,并伴随45%(VPGM=4 V)更低的畴响应分布系数 |
| 正交相晶粒 | o相分数+44%、晶粒大20 nm、粗糙度Rq降低75% | 赝形模板促进o相成核与均匀生长,o相晶粒超过25 nm |
2Pr = 133 μC/cm²;Ec = 1.17 MV/cm(6 nm HZO)
铁电极化、原子层沉积(ALD)、神经形态、存内计算、模拟权重
低功耗铁电存储器(FeRAM)、神经形态计算/二值神经网络推理、CMOS兼容嵌入式存储